PA15um/CPE80um white bag, boiling-resistant adhesive 3gm, delaminates when rubbed by hand, why?

Published:2017-08-10 · Industry News · Source: 包装前沿
Key Takeaways
  • The case is a PA15μm/CPE80μm white bag using 3 g/m² boil-resistant adhesive, cured at 38–40°C for 24 h, with poor lamination strength and hand-rub delamination after bag-making.
  • The discussion recommended dry-lamination curing normally at 50–55°C, with boil/retort curing around 50°C, and considered 38–40°C low and 24 h short.
  • Comments pointed to excessive PE additive/slip-agent exudation or too much PE powder, said additive exudation has little to do with corona, and Jin’s corona-pen test showed no corona problem.
  • For a 3 g/m² coating weight, a 120-line anilox was considered basically sufficient, the 170-line anilox and high viscosity were questioned, and a heat-sealer test was suggested to check strength changes.
  • Adding two more days of curing did not help, and finished bags on an 80°C hot drum could not be peeled apart after 1 minute.

Jin: PA15um/CPE80um white bag, boiling-resistant adhesive 3gsm, curing room at 38~40℃ for 24h; when taken out to make bags, the lamination strength between the two films is poor, and it delaminates when rubbed by hand. Why? Harbin Botai - Chen: Downward-blown PE? Jin: Cast film. Harbin Botai - Chen: The curing temperature for dry lamination is a bit low; it should normally be 50~55℃. Jin: We never had this situation before. Does such a high temperature affect heat sealing? Harbin Botai - Chen: Will it be tacky after separation? Jin: No. Hangzhou Flexible Packaging - Xiao Chen: The curing time in the curing room is also a bit short. Packaging Corner Missing: PE corona problem. Hangzhou Flexible Packaging - Xiao Chen: Generally, boiling or retort curing is at around 50℃. Fujian Enterprise Management - Zhou: This is clearly caused by too much exudate. Jin: Later I put it back to cure for two days, but it didn't help. No boiling is needed, just vacuum. Shanghai Yida Dry Lamination: Your PE has powder. Hangzhou Flexible Packaging - Xiao Chen: Then consider slip agent exudation from the CPE. Jin: I tested it with a corona pen; there is no problem. Hangzhou Flexible Packaging - Xiao Chen: If it is additive exudation, it has little to do with corona. Shanghai Yida Dry Lamination: It is caused by powder on your PE and too much powder; it has nothing to do with corona. Jin: I didn't notice powder on the PE; I suspect that too. This batch of film is hard and bright. Shanghai Yida Dry Lamination: It is caused by too many additives in the PE. Harbin Botai - Chen: To prevent slip agent exudation from PE, it is best to cure at high temperature first. Plastic Color Printing Food Packaging: What is the anilox line count? Jin: 170. Harbin Botai - Chen: Can 170 transfer 3 g/m2? Plastic Color Printing Food Packaging: Should use 120. Jin: The viscosity is very high. Hangzhou Flexible Packaging - Xiao Chen: For a coating weight of 3 g/m2, a 120-line anilox is basically enough. Harbin Botai - Chen: I suggest you seal it with a heat sealer and then see whether the strength changes? Jin: We have even used 200 before. Shanghai Yida Dry Lamination: Even if you change the PA and laminate that PE again, it still won't bond well. Harbin Botai - Chen: The strength is good, but there is too much exudate; the curing temperature is low. Jin: When the finished bags are placed on an 80℃ hot drum, they cannot be peeled apart after one minute. Shanghai Yida Dry Lamination: I had this problem before too; change the PE. Harbin Botai - Chen: This is a race between exudation time and curing time; first cure at 55℃ for 10~12h, then lower it to around 50℃. Plastic Color Printing Food Packaging: If the product has not entered the curing oven, it will definitely be tacky. Jin: There is none. We have run a ton of material and made half of the bags. What should we do? Hangzhou Flexible Packaging - Xiao Chen: It has already exuded now; further curing will probably have little effect. Jin: Does the oven temperature for PE film need to be this high? Foshan Packaging: Try an adhesive with low extraction of exudates. Beijing - Engineer Li: Curing above 70℃ for more than 12h may be better. Jin: Are the finished ones still usable? Foshan Packaging: No use; re-curing only gives a false increase, and it drops again after cooling. Jin: Then what should we do? The same process never had this problem before. Hangzhou Flexible Packaging - Xiao Chen: Peel it open and see whether there is white exudate on the CPE that can be wiped off by hand. Plastic Color Printing Food Packaging: Replace the PE. Foshan Packaging: Actually, solventless adhesive extracts much less PE exudate than dry lamination, and the coating weight does not need to be deliberately increased. Jin: There is white exudate. Hangzhou Flexible Packaging - Xiao Chen: Then it is a CPE problem. Foshan Packaging: Change the PE or the adhesive. Hunan - Changsha - Xiao Zhang: Slip agent exudation. Fujian Enterprise Management - Zhou: If it can be fully delaminated, use a slitter to delaminate the rest, adjust after rewinding, and laminate once more to reduce losses. Jin: Can the PA still be used? Fujian Enterprise Management - Zhou: Yes, it can. Jin: Okay, thank you everyone. (If you have different opinions, you are welcome to continue the discussion at www.pack168.com. Friends who provide more solutions can receive reading points for technical articles on the website. To request points, please contact Xiaoyang: 15813331361, Xiaolai: 18475695660)

Related reading

  • From Sorting Lines to Freeze-drying Workshops · …
    2026-11-27Industry NewsSource: 食品机械设备网·资讯

    Sichuan and Chongqing are major domestic lemon producing regions, with Anyue in Sichuan and Tongnan in Chongqing being widely renowned. For a long period, however, most lemons from the two regions were sold outward as fresh fruits, with their size and skin appearance directly determining the selling price. The proportion of deep processing was low, and processing lemons of ordinary appearance could often only be sold at low prices, or even rot in the fields. The key to generating higher added value from small lemons lies in deep processing, and every link of this chain cannot function without the support of food machinery. Sorting and Grading: First Divide Raw Materials

  • Consumer Environment Optimization Month | Tips for Purchasing and Using Plastic Food-related Products
    2026-11-26Industry NewsSource: 食品伙伴网

    Plastic food-related products refer to products such as plastic packaging, containers and tools that take resin or thermoplastic materials as the main raw materials, are used to package and hold food or food additives, and come into direct contact with food during food production and operation. China implements production license management for food-use plastic packaging, containers, tools and other products, and enterprises shall obtain a production license before engaging in production and operation. Common plastic food-related products used by consumers include melamine tableware, disposable plastic

  • UPM Strengthens Label Materials Capacity in Asia Pacific
    2026-11-26Industry NewsSource: Packaging News Australia

    UPM Adhesive Materials has completed a major investment in its label materials factory in Johor Bahru, Malaysia, increasing capacity and efficiency to support growth in Asia Pacific. The upgraded factory features an advanced coating line and enhanced post-processing, packing, and material handling capabilities.

  • Intelligence Empowers Industry · Industry-innovation Collaboration | The AI Special Session of the 2026 · …
    2026-11-24Industry NewsSource: 食品机械设备网

    From November 17 to 18, the AI Special Session of the 2026 Industry-innovation Collaborative Innovation Event, hosted by the China Association for Science and Technology and the All-China Federation of Industry and Commerce, undertaken by the Enterprise Innovation Service Center of the China Association for Science and Technology, the Publicity and Education Department and the Economic Service Department of the All-China Federation of Industry and Commerce, and implemented by the Guangdong Food and Packaging Machinery Industry Association, the Guangzhou Food and Packaging Industry Enterprise Science Association Federation jointly with multiple enterprises and institutions, was held at the Meilihao Hotel in Panyu, Guangzhou. This event takes the theme of "

Contact us for a quote

For samples, pricing or technical support, call us or leave a message and we will reply shortly.

+86 15916881866 Contact us