PA15μm/CPE80μmの白袋、耐煮沸性接着剤3g/m²、手でこすると層間剥離するのはなぜですか?
- 该案例为PA15μm/CPE80μm白色袋,使用耐煮胶3g/m²,在38~40℃熟化24h后制袋,两层膜复合强度差且手搓即分层。
- 讨论中建议干式复合熟化温度通常应为50~55℃、耐煮/蒸煮熟化约50℃,并认为38~40℃偏低且24h偏短。
- 有观点将问题指向PE添加剂/滑爽剂析出过多或PE粉过多,认为添加剂析出与电晕关系不大,而提问者用达因笔测试未发现电晕问题。
- 在3g/m²涂布量下,讨论认为120线网纹辊基本够用,并对170线网纹辊及高粘度提出疑问,建议用热封机测试强度变化。
- 后续再熟化两天仍未改善,且成品袋放在80℃热鼓上1分钟不能剥离。
Jin: PA15um/CPE80um white bag, boiling-resistant adhesive 3gsm, curing room at 38~40℃ for 24h; when taken out to make bags, the lamination strength between the two films is poor, and it delaminates when rubbed by hand. Why? Harbin Botai - Chen: Downward-blown PE? Jin: Cast film. Harbin Botai - Chen: The curing temperature for dry lamination is a bit low; it should normally be 50~55℃. Jin: We never had this situation before. Does such a high temperature affect heat sealing? Harbin Botai - Chen: Will it be tacky after separation? Jin: No. Hangzhou Flexible Packaging - Xiao Chen: The curing time in the curing room is also a bit short. Packaging Corner Missing: PE corona problem. Hangzhou Flexible Packaging - Xiao Chen: Generally, boiling or retort curing is at around 50℃. Fujian Enterprise Management - Zhou: This is clearly caused by too much exudate. Jin: Later I put it back to cure for two days, but it didn't help. No boiling is needed, just vacuum. Shanghai Yida Dry Lamination: Your PE has powder. Hangzhou Flexible Packaging - Xiao Chen: Then consider slip agent exudation from the CPE. Jin: I tested it with a corona pen; there is no problem. Hangzhou Flexible Packaging - Xiao Chen: If it is additive exudation, it has little to do with corona. Shanghai Yida Dry Lamination: It is caused by powder on your PE and too much powder; it has nothing to do with corona. Jin: I didn't notice powder on the PE; I suspect that too. This batch of film is hard and bright. Shanghai Yida Dry Lamination: It is caused by too many additives in the PE. Harbin Botai - Chen: To prevent slip agent exudation from PE, it is best to cure at high temperature first. Plastic Color Printing Food Packaging: What is the anilox line count? Jin: 170. Harbin Botai - Chen: Can 170 transfer 3 g/m2? Plastic Color Printing Food Packaging: Should use 120. Jin: The viscosity is very high. Hangzhou Flexible Packaging - Xiao Chen: For a coating weight of 3 g/m2, a 120-line anilox is basically enough. Harbin Botai - Chen: I suggest you seal it with a heat sealer and then see whether the strength changes? Jin: We have even used 200 before. Shanghai Yida Dry Lamination: Even if you change the PA and laminate that PE again, it still won't bond well. Harbin Botai - Chen: The strength is good, but there is too much exudate; the curing temperature is low. Jin: When the finished bags are placed on an 80℃ hot drum, they cannot be peeled apart after one minute. Shanghai Yida Dry Lamination: I had this problem before too; change the PE. Harbin Botai - Chen: This is a race between exudation time and curing time; first cure at 55℃ for 10~12h, then lower it to around 50℃. Plastic Color Printing Food Packaging: If the product has not entered the curing oven, it will definitely be tacky. Jin: There is none. We have run a ton of material and made half of the bags. What should we do? Hangzhou Flexible Packaging - Xiao Chen: It has already exuded now; further curing will probably have little effect. Jin: Does the oven temperature for PE film need to be this high? Foshan Packaging: Try an adhesive with low extraction of exudates. Beijing - Engineer Li: Curing above 70℃ for more than 12h may be better. Jin: Are the finished ones still usable? Foshan Packaging: No use; re-curing only gives a false increase, and it drops again after cooling. Jin: Then what should we do? The same process never had this problem before. Hangzhou Flexible Packaging - Xiao Chen: Peel it open and see whether there is white exudate on the CPE that can be wiped off by hand. Plastic Color Printing Food Packaging: Replace the PE. Foshan Packaging: Actually, solventless adhesive extracts much less PE exudate than dry lamination, and the coating weight does not need to be deliberately increased. Jin: There is white exudate. Hangzhou Flexible Packaging - Xiao Chen: Then it is a CPE problem. Foshan Packaging: Change the PE or the adhesive. Hunan - Changsha - Xiao Zhang: Slip agent exudation. Fujian Enterprise Management - Zhou: If it can be fully delaminated, use a slitter to delaminate the rest, adjust after rewinding, and laminate once more to reduce losses. Jin: Can the PA still be used? Fujian Enterprise Management - Zhou: Yes, it can. Jin: Okay, thank you everyone. (If you have different opinions, you are welcome to continue the discussion at www.pack168.com. Friends who provide more solutions can receive reading points for technical articles on the website. To request points, please contact Xiaoyang: 15813331361, Xiaolai: 18475695660)
関連資料
- 選果ラインから凍結乾燥工場まで:食品機械が紡ぐ四川・重慶レモンの深加工チェーン2026-11-27Industry Newsソース: 食品机械设备网·资讯
四川省と重慶市は中国国内の主要なレモン産地であり、中でも四川省安岳県と重慶市潼南区は広く知られている。しかし長らくの間、両地域のレモンの多くは青果として域外に販売され、そのサイズと果皮の外観が販売価格を直接左右していた。深加工の割合は低く、外観が平均的な加工用レモンは低価格でしか販売できないことが多く、ひどい場合には畑で腐ってしまうことさえあった。 小さなレモンからより高い付加価値を生み出す鍵は深加工にあり、このチェーンのあらゆる工程には食品機械のサポートが欠かせません。選別・等級分け:まず原材料を区分する
- 消費者向け環境最適化月間|プラスチック製食品関連製品の購入・使用のヒント2026-11-26Industry Newsソース: 食品伙伴网
食品関連プラスチック製品とは、樹脂または熱可塑性材料を主原料とし、食品や食品添加物の包装・保持に使用され、食品の生産・販売過程において食品に直接接触する製品をいう。中国では、食品用プラスチック包装、容器、工具などの製品に生産許可制度を適用しており、企業は生産・販売活動を開始する前に生産許可証を取得しなければならない。 消費者が利用する一般的なプラスチック製食品関連製品には、メラミン製食器、使い捨てプラスチック製品などがある
- UPM、アジア太平洋地域のラベル材料の生産能力を増強2026-11-26Industry Newsソース: Packaging News Australia
UPM Adhesive Materialsは、マレーシアのジョホールバルにあるラベル材料工場への大規模投資を完了し、アジア太平洋地域での成長を支えるため、生産能力と効率を向上させました。改修された工場には、先進的なコーティングラインが導入され、後加工、梱包、materials搬送能力が強化されています。
- 知能が産業をエンパワー・産学連携イノベーション|2026年産学連携イノベーションイベントAI特別セッションが広州で開催2026-11-24Industry Newsソース: 食品机械设备网
11月17日から18日まで、中国科学技術協会と中華全国工商業連合会が主催し、中国科学技術協会企業革新サービスセンター、中華全国工商業連合会宣伝教育部・経済サービス部が運営を担い、広東省食品・包装機械工業協会、広州市食品・包装業企業科学協会連合会が複数の企業・機関と共同で実施した2026年産業イノベーション協働革新イベントのAI特別セッションが、広州番禺のメリハオホテルで開催された。本イベントは「