  • 该案例为PA15μm/CPE80μm白色袋,使用耐煮胶3g/m²,在38~40℃熟化24h后制袋,两层膜复合强度差且手搓即分层。
  • 讨论中建议干式复合熟化温度通常应为50~55℃、耐煮/蒸煮熟化约50℃,并认为38~40℃偏低且24h偏短。
  • 有观点将问题指向PE添加剂/滑爽剂析出过多或PE粉过多,认为添加剂析出与电晕关系不大,而提问者用达因笔测试未发现电晕问题。
  • 在3g/m²涂布量下,讨论认为120线网纹辊基本够用,并对170线网纹辊及高粘度提出疑问,建议用热封机测试强度变化。
  • 后续再熟化两天仍未改善,且成品袋放在80℃热鼓上1分钟不能剥离。

Jin: PA15um/CPE80um white bag, boiling-resistant adhesive 3gsm, curing room at 38~40℃ for 24h; when taken out to make bags, the lamination strength between the two films is poor, and it delaminates when rubbed by hand. Why? Harbin Botai - Chen: Downward-blown PE? Jin: Cast film. Harbin Botai - Chen: The curing temperature for dry lamination is a bit low; it should normally be 50~55℃. Jin: We never had this situation before. Does such a high temperature affect heat sealing? Harbin Botai - Chen: Will it be tacky after separation? Jin: No. Hangzhou Flexible Packaging - Xiao Chen: The curing time in the curing room is also a bit short. Packaging Corner Missing: PE corona problem. Hangzhou Flexible Packaging - Xiao Chen: Generally, boiling or retort curing is at around 50℃. Fujian Enterprise Management - Zhou: This is clearly caused by too much exudate. Jin: Later I put it back to cure for two days, but it didn't help. No boiling is needed, just vacuum. Shanghai Yida Dry Lamination: Your PE has powder. Hangzhou Flexible Packaging - Xiao Chen: Then consider slip agent exudation from the CPE. Jin: I tested it with a corona pen; there is no problem. Hangzhou Flexible Packaging - Xiao Chen: If it is additive exudation, it has little to do with corona. Shanghai Yida Dry Lamination: It is caused by powder on your PE and too much powder; it has nothing to do with corona. Jin: I didn't notice powder on the PE; I suspect that too. This batch of film is hard and bright. Shanghai Yida Dry Lamination: It is caused by too many additives in the PE. Harbin Botai - Chen: To prevent slip agent exudation from PE, it is best to cure at high temperature first. Plastic Color Printing Food Packaging: What is the anilox line count? Jin: 170. Harbin Botai - Chen: Can 170 transfer 3 g/m2? Plastic Color Printing Food Packaging: Should use 120. Jin: The viscosity is very high. Hangzhou Flexible Packaging - Xiao Chen: For a coating weight of 3 g/m2, a 120-line anilox is basically enough. Harbin Botai - Chen: I suggest you seal it with a heat sealer and then see whether the strength changes? Jin: We have even used 200 before. Shanghai Yida Dry Lamination: Even if you change the PA and laminate that PE again, it still won't bond well. Harbin Botai - Chen: The strength is good, but there is too much exudate; the curing temperature is low. Jin: When the finished bags are placed on an 80℃ hot drum, they cannot be peeled apart after one minute. Shanghai Yida Dry Lamination: I had this problem before too; change the PE. Harbin Botai - Chen: This is a race between exudation time and curing time; first cure at 55℃ for 10~12h, then lower it to around 50℃. Plastic Color Printing Food Packaging: If the product has not entered the curing oven, it will definitely be tacky. Jin: There is none. We have run a ton of material and made half of the bags. What should we do? Hangzhou Flexible Packaging - Xiao Chen: It has already exuded now; further curing will probably have little effect. Jin: Does the oven temperature for PE film need to be this high? Foshan Packaging: Try an adhesive with low extraction of exudates. Beijing - Engineer Li: Curing above 70℃ for more than 12h may be better. Jin: Are the finished ones still usable? Foshan Packaging: No use; re-curing only gives a false increase, and it drops again after cooling. Jin: Then what should we do? The same process never had this problem before. Hangzhou Flexible Packaging - Xiao Chen: Peel it open and see whether there is white exudate on the CPE that can be wiped off by hand. Plastic Color Printing Food Packaging: Replace the PE. Foshan Packaging: Actually, solventless adhesive extracts much less PE exudate than dry lamination, and the coating weight does not need to be deliberately increased. Jin: There is white exudate. Hangzhou Flexible Packaging - Xiao Chen: Then it is a CPE problem. Foshan Packaging: Change the PE or the adhesive. Hunan - Changsha - Xiao Zhang: Slip agent exudation. Fujian Enterprise Management - Zhou: If it can be fully delaminated, use a slitter to delaminate the rest, adjust after rewinding, and laminate once more to reduce losses. Jin: Can the PA still be used? Fujian Enterprise Management - Zhou: Yes, it can. Jin: Okay, thank you everyone. (If you have different opinions, you are welcome to continue the discussion at www.pack168.com. Friends who provide more solutions can receive reading points for technical articles on the website. To request points, please contact Xiaoyang: 15813331361, Xiaolai: 18475695660)

Bacaan terkait

  • Dari Jalur Penyortiran hingga Bengkel Pengeringan Beku · …
    2026-11-27Industry NewsSumber: 食品机械设备网·资讯

    Sichuan dan Chongqing merupakan wilayah penghasil lemon utama di dalam negeri, di mana Anyue di Sichuan dan Tongnan di Chongqing sangat terkenal. Namun, dalam jangka waktu yang lama, sebagian besar lemon dari kedua wilayah tersebut dijual ke luar sebagai buah segar, dengan ukuran dan tampilan kulit secara langsung menentukan harga jual. Proporsi pengolahan mendalam masih rendah, dan lemon dengan tampilan biasa yang diolah seringkali hanya dapat dijual dengan harga murah, bahkan membusuk di ladang. Kunci untuk menghasilkan nilai tambah yang lebih tinggi dari lemon kecil terletak pada pemrosesan mendalam, dan setiap tautan dalam rantai ini tidak dapat berfungsi tanpa dukungan mesin makanan. Penyortiran dan Penggolongan: Bagi Bahan Baku Terlebih Dahulu

  • Bulan Optimalisasi Lingkungan Konsumen | Tips Membeli dan Menggunakan Produk Plastik untuk Kemasan Makanan
    2026-11-26Industry NewsSumber: 食品伙伴网

    Produk plastik terkait makanan mencakup produk seperti kemasan plastik, wadah, dan alat yang menggunakan resin atau material termoplastik sebagai bahan baku utama, digunakan untuk mengemas dan menampung makanan atau aditif makanan, serta bersentuhan langsung dengan makanan selama proses produksi dan operasional. China menerapkan manajemen izin produksi untuk kemasan plastik untuk makanan, wadah, alat, dan produk lainnya, dan perusahaan harus memperoleh izin produksi sebelum melakukan produksi dan operasional. Produk plastik terkait makanan yang umum digunakan konsumen mencakup peralatan makan dari melamin, plastik sekali pakai

  • UPM Perkuat Kapasitas Produksi Material Label di Asia Pasifik
    2026-11-26Industry NewsSumber: Packaging News Australia

    UPM Adhesive Materials telah melakukan investasi besar di pabrik bahan labelnya di Johor Bahru, Malaysia, dengan meningkatkan kapasitas dan efisiensi untuk mendukung pertumbuhan di Asia Pasifik. Pabrik yang telah ditingkatkan ini dilengkapi lini pelapisan mutakhir serta kemampuan pascaproses, pengemasan, dan penanganan material yang lebih baik.

  • Kecerdasan Buatan Memberdayakan Industri · Kolaborasi Inovasi Industri | Sesi Khusus AI Acara Inovasi · …
    2026-11-24Industry NewsSumber: 食品机械设备网

    Dari 17 hingga 18 November, Sesi Khusus AI dari Kegiatan Inovasi Kolaboratif Inovasi Industri 2026, yang diselenggarakan oleh Asosiasi Ilmu Pengetahuan dan Teknologi Tiongkok serta Federasi Industri dan Perdagangan Seluruh Tiongkok, yang dilaksanakan oleh Pusat Layanan Inovasi Perusahaan Asosiasi Ilmu Pengetahuan dan Teknologi Tiongkok, Departemen Publisitas dan Pendidikan serta Departemen Layanan Ekonomi Federasi Industri dan Perdagangan Seluruh Tiongkok, dan diimplementasikan oleh Asosiasi Industri Mesin Makanan dan Kemasan Guangdong, Federasi Asosiasi Ilmu Pengetahuan Perusahaan Industri Makanan dan Kemasan Guangzhou bersama dengan beberapa perusahaan dan institusi, diadakan di Hotel Meilihao, Panyu, Guangzhou. Acara ini mengusung tema "

Hubungi kami untuk mendapatkan penawaran

Untuk sampel, harga, atau dukungan teknis, hubungi kami atau tinggalkan pesan dan kami akan segera membalas.

+86 15916881866 Hubungi kami