콘크리트 면 댐 워터스톱: SR 플라스틱 충전재, GB 유연 충전재 및 EPDM 복합 커버 플레이트 시공 안내서
- 对于混凝土面板坝的二次止水系统,施工指南涉及SR塑性填料、GB柔性填料和EPDM复合盖板,安装在水轮趾板与面板之间的止水槽整平及波纹止水安装之后进行。
- 氯丁橡胶棒采用对接连接,接头用胶粘剂和胶带加固,并用细铅丝将其固定在槽内的沥青杉木板中,以防止滑移或位移。
- 关键安装控制点包括保持界面清洁干燥、确保填料层之间及填料与混凝土之间密实粘结,以及EPDM盖板与混凝土基面牢固粘附;干燥混凝土使用干型胶粘剂,潮湿区域先干燥再使用湿面胶粘剂。
- 填料施工时,一块填料先分成两半放在槽底并压紧粘结,随后逐层从中部向两侧粘结并排出空气,填料接缝搭接;EPDM盖板沿填料中心线对称放置,并用橡胶锤敲实。
- 安装EPDM盖板前,应每10–20米进行破坏性检查,检查填料层间是否存在气泡或杂物,并核对与混凝土基面的粘结面积比;若粘结面积比低于规定要求,该段必须返工。
SR plastic filler, GB flexible filler, and EPDM composite cover plate
Installation method for EPDM composite cover plates
Construction process for plastic filler
Within the secondary waterstop system of concrete face dams, this step plays a central role
The anti-seepage cover sheet creates a complete waterproofing system
and is essential to the safe operation of the face dam.
However, on real projects, filler application still faces practical issues
Many construction teams are not fully familiar with the material
and have limited knowledge of the detailed installation steps
After the waterstop groove between the plinth and the face slab is leveled
the corrugated waterstop is then installed
Neoprene rods are connected in a butt joint
Joints are reinforced with adhesive and tape
To prevent slipping or displacement
fine lead wire is used to secure them to the asphalt cedar board inside the groove.
During the installation of filler and EPDM cover plates
the key control points are
keeping the interface clean and dry
ensuring dense bonding between filler layers and between filler and concrete
and achieving firm adhesion between the EPDM cover plate and the concrete substrate
During work, the interface is first roughened and cleaned with an angle grinder and wire brush
then wiped clean with cotton yarn
For wet or damp areas
dry them first and then apply a wet-surface adhesive
On dry concrete surfaces, a dry-type adhesive is applied
Dry-type adhesive generally needs to be left to dry
The open time depends on temperature, wind speed, and other factors
It is ready for covering when it feels tacky but does not stick to the hand
Wet-surface adhesive does not require drying and can be covered directly with filler.
During application, the release paper is removed from the packaging
A piece of filler is first split into two halves
and placed at the bottom of the groove
Pressure is applied to bond it firmly
Additional layers are then bonded one by one
working from the center toward both sides for a dense bond
Air is expelled while bonding
Filler joints are overlapped
so that the filler and interface form a dense, integrated whole.
Before installing the EPDM cover plate, inspect
the quality of the filler installation
At 10–20 m intervals
perform a destructive check
Open up the completed section
and check for air pockets or debris between filler layers
verify whether bonding is tight
Also check the bonded area ratio against the concrete substrate
If the bonded area ratio is lower than
the specified requirement, the section must be reworked
The cover plate is placed symmetrically along the filler centerline
and pressed gradually from the center toward both sides
A rubber mallet is used to tamp it down
to drive out trapped air
This creates a tight bond between the filler and the EPDM cover plate.
The edge area where the cover plate bonds to the concrete substrate must first be treated according to the process
This helps the cover plate adhere more tightly and securely to the concrete surface.
EPDM composite cover plate
Joints between cover plates are handled as butt joints
At the lap area
primer is applied to the filler, then a piece is laid over it
The cover plate is then placed neatly over the composite board
and tapped tight with a rubber mallet.
The original EPDM cover plate fixing design used, on both sides,
unequal angle steel with expansion bolts
Because the concrete surfaces on both sides of the cover plate cannot be perfectly uniform
angle steel is highly rigid
and cannot accommodate such deformation
The original angle steel specification was therefore changed
The result improved to a certain extent
but more joints were added
and the joint areas were difficult to compact
After a design revision, the angle steel was replaced with an alternative solution
Source: China Packaging Network (pack.cn); original link: http://news.pack.cn/show-345672.html
관련 읽기
- 선별 라인부터 동결건조 작업장까지: 식품 기계가 엮어가는 쓰촨·충칭 레몬 심층 가공 체인2026-11-27Industry News출처: 食品机械设备网·资讯
쓰촨성과 충칭시는 국내 주요 레몬 생산지로, 특히 쓰촨성 안웨현과 충칭시 퉁난구는 널리 알려져 있습니다. 하지만 오랫동안 두 지역의 레몬 대부분은 생과일로 외부에 판매되었으며, 과일의 크기와 껍질 상태가 판매 가격을 직접 결정했습니다. 심층 가공 비중이 낮았고, 외관이 평범한 가공용 레몬은 대부분 저가로 판매되거나 심지어 밭에서 썩어가는 경우도 많았습니다. 작은 레몬으로 더 높은 부가가치를 창출하는 핵심은 심층 가공에 있으며, 이 가공 사슬의 모든 단계는 식품 기계의 지원 없이 운영될 수 없습니다. 선별 및 등급 분류: 원료를 먼저 나누기
- 소비자 환경 최적화 달 | 플라스틱 식품용 제품 구매 및 사용 팁2026-11-26Industry News출처: 食品伙伴网
플라스틱 식품 관련 제품은 수지 또는 열가소성 재료를 주원료로 사용하여 식품 또는 식품 첨가물을 포장·보관하고, 식품 생산 및 영업 과정에서 식품과 직접 접촉하는 플라스틱 포장, 용기, 공구 등의 제품이다. 중국은 식품용 플라스틱 포장, 용기, 공구 및 기타 제품에 대해 생산허가 관리를 시행하며, 기업은 생산 및 영업에 착수하기 전에 생산허가를 취득해야 한다. 소비자들이 사용하는 일반적인 플라스틱 식품 관련 제품에는 멜라민 식기, 일회용 플라스틱이 포함됩니다
- UPM, 아시아태평양 지역 라벨 소재 생산능력 강화2026-11-26Industry News출처: Packaging News Australia
UPM Adhesive Materials는 말레이시아 조호바루의 라벨용 소재 공장에 대규모 투자를 완료해 생산능력과 효율을 높이고 아태 지역의 성장을 지원했습니다. 현대화된 공장에는 최신식 코팅 라인과 강화된 후처리, 포장 및 자재 취급 설비가 갖춰져 있습니다.
- 지능이 산업에 힘을 실어주다 · 산업-혁신 협업 | 2026 산업-혁신 협력 혁신 행사 AI 특별 세션, 광저우에서 개최2026-11-24Industry News출처: 食品机械设备网
11월 17일부터 18일까지 중국과학기술협회와 중국전국공상업연합회가 주최하고 중국과학기술협회 기업혁신서비스센터, 중국전국공상업연합회 홍보교육부·경제서비스부가 주관하며 광둥성 식품 및 포장 기계 산업 협회, 광저우 식품 및 포장 산업 기업 과학 협회 연합회가 여러 기업 및 기관과 공동으로 시행한 2026 산업 혁신 협력 혁신 행사의 AI 특별 세션이 광저우 판위에 위치한 메이리하오 호텔에서 개최되었습니다. 이번 행사는 "을 주제로 합니다