Waterstop Bendungan Muka Beton: Panduan Konstruksi SR Plastic Filler, GB Flexible Filler dan Pelat Penutup Komposit EPDM
- 对于混凝土面板坝的二次止水系统,施工指南涉及SR塑性填料、GB柔性填料和EPDM复合盖板,安装在水轮趾板与面板之间的止水槽整平及波纹止水安装之后进行。
- 氯丁橡胶棒采用对接连接,接头用胶粘剂和胶带加固,并用细铅丝将其固定在槽内的沥青杉木板中,以防止滑移或位移。
- 关键安装控制点包括保持界面清洁干燥、确保填料层之间及填料与混凝土之间密实粘结,以及EPDM盖板与混凝土基面牢固粘附;干燥混凝土使用干型胶粘剂,潮湿区域先干燥再使用湿面胶粘剂。
- 填料施工时,一块填料先分成两半放在槽底并压紧粘结,随后逐层从中部向两侧粘结并排出空气,填料接缝搭接;EPDM盖板沿填料中心线对称放置,并用橡胶锤敲实。
- 安装EPDM盖板前,应每10–20米进行破坏性检查,检查填料层间是否存在气泡或杂物,并核对与混凝土基面的粘结面积比;若粘结面积比低于规定要求,该段必须返工。
SR plastic filler, GB flexible filler, and EPDM composite cover plate
Installation method for EPDM composite cover plates
Construction process for plastic filler
Within the secondary waterstop system of concrete face dams, this step plays a central role
The anti-seepage cover sheet creates a complete waterproofing system
and is essential to the safe operation of the face dam.
However, on real projects, filler application still faces practical issues
Many construction teams are not fully familiar with the material
and have limited knowledge of the detailed installation steps
After the waterstop groove between the plinth and the face slab is leveled
the corrugated waterstop is then installed
Neoprene rods are connected in a butt joint
Joints are reinforced with adhesive and tape
To prevent slipping or displacement
fine lead wire is used to secure them to the asphalt cedar board inside the groove.
During the installation of filler and EPDM cover plates
the key control points are
keeping the interface clean and dry
ensuring dense bonding between filler layers and between filler and concrete
and achieving firm adhesion between the EPDM cover plate and the concrete substrate
During work, the interface is first roughened and cleaned with an angle grinder and wire brush
then wiped clean with cotton yarn
For wet or damp areas
dry them first and then apply a wet-surface adhesive
On dry concrete surfaces, a dry-type adhesive is applied
Dry-type adhesive generally needs to be left to dry
The open time depends on temperature, wind speed, and other factors
It is ready for covering when it feels tacky but does not stick to the hand
Wet-surface adhesive does not require drying and can be covered directly with filler.
During application, the release paper is removed from the packaging
A piece of filler is first split into two halves
and placed at the bottom of the groove
Pressure is applied to bond it firmly
Additional layers are then bonded one by one
working from the center toward both sides for a dense bond
Air is expelled while bonding
Filler joints are overlapped
so that the filler and interface form a dense, integrated whole.
Before installing the EPDM cover plate, inspect
the quality of the filler installation
At 10–20 m intervals
perform a destructive check
Open up the completed section
and check for air pockets or debris between filler layers
verify whether bonding is tight
Also check the bonded area ratio against the concrete substrate
If the bonded area ratio is lower than
the specified requirement, the section must be reworked
The cover plate is placed symmetrically along the filler centerline
and pressed gradually from the center toward both sides
A rubber mallet is used to tamp it down
to drive out trapped air
This creates a tight bond between the filler and the EPDM cover plate.
The edge area where the cover plate bonds to the concrete substrate must first be treated according to the process
This helps the cover plate adhere more tightly and securely to the concrete surface.
EPDM composite cover plate
Joints between cover plates are handled as butt joints
At the lap area
primer is applied to the filler, then a piece is laid over it
The cover plate is then placed neatly over the composite board
and tapped tight with a rubber mallet.
The original EPDM cover plate fixing design used, on both sides,
unequal angle steel with expansion bolts
Because the concrete surfaces on both sides of the cover plate cannot be perfectly uniform
angle steel is highly rigid
and cannot accommodate such deformation
The original angle steel specification was therefore changed
The result improved to a certain extent
but more joints were added
and the joint areas were difficult to compact
After a design revision, the angle steel was replaced with an alternative solution
Source: China Packaging Network (pack.cn); original link: http://news.pack.cn/show-345672.html
Bacaan terkait
- Dari Jalur Penyortiran hingga Bengkel Pengeringan Beku · …2026-11-27Industry NewsSumber: 食品机械设备网·资讯
Sichuan dan Chongqing merupakan wilayah penghasil lemon utama di dalam negeri, di mana Anyue di Sichuan dan Tongnan di Chongqing sangat terkenal. Namun, dalam jangka waktu yang lama, sebagian besar lemon dari kedua wilayah tersebut dijual ke luar sebagai buah segar, dengan ukuran dan tampilan kulit secara langsung menentukan harga jual. Proporsi pengolahan mendalam masih rendah, dan lemon dengan tampilan biasa yang diolah seringkali hanya dapat dijual dengan harga murah, bahkan membusuk di ladang. Kunci untuk menghasilkan nilai tambah yang lebih tinggi dari lemon kecil terletak pada pemrosesan mendalam, dan setiap tautan dalam rantai ini tidak dapat berfungsi tanpa dukungan mesin makanan. Penyortiran dan Penggolongan: Bagi Bahan Baku Terlebih Dahulu
- Bulan Optimalisasi Lingkungan Konsumen | Tips Membeli dan Menggunakan Produk Plastik untuk Kemasan Makanan2026-11-26Industry NewsSumber: 食品伙伴网
Produk plastik terkait makanan mencakup produk seperti kemasan plastik, wadah, dan alat yang menggunakan resin atau material termoplastik sebagai bahan baku utama, digunakan untuk mengemas dan menampung makanan atau aditif makanan, serta bersentuhan langsung dengan makanan selama proses produksi dan operasional. China menerapkan manajemen izin produksi untuk kemasan plastik untuk makanan, wadah, alat, dan produk lainnya, dan perusahaan harus memperoleh izin produksi sebelum melakukan produksi dan operasional. Produk plastik terkait makanan yang umum digunakan konsumen mencakup peralatan makan dari melamin, plastik sekali pakai
- UPM Perkuat Kapasitas Produksi Material Label di Asia Pasifik2026-11-26Industry NewsSumber: Packaging News Australia
UPM Adhesive Materials telah melakukan investasi besar di pabrik bahan labelnya di Johor Bahru, Malaysia, dengan meningkatkan kapasitas dan efisiensi untuk mendukung pertumbuhan di Asia Pasifik. Pabrik yang telah ditingkatkan ini dilengkapi lini pelapisan mutakhir serta kemampuan pascaproses, pengemasan, dan penanganan material yang lebih baik.
- Kecerdasan Buatan Memberdayakan Industri · Kolaborasi Inovasi Industri | Sesi Khusus AI Acara Inovasi · …2026-11-24Industry NewsSumber: 食品机械设备网
Dari 17 hingga 18 November, Sesi Khusus AI dari Kegiatan Inovasi Kolaboratif Inovasi Industri 2026, yang diselenggarakan oleh Asosiasi Ilmu Pengetahuan dan Teknologi Tiongkok serta Federasi Industri dan Perdagangan Seluruh Tiongkok, yang dilaksanakan oleh Pusat Layanan Inovasi Perusahaan Asosiasi Ilmu Pengetahuan dan Teknologi Tiongkok, Departemen Publisitas dan Pendidikan serta Departemen Layanan Ekonomi Federasi Industri dan Perdagangan Seluruh Tiongkok, dan diimplementasikan oleh Asosiasi Industri Mesin Makanan dan Kemasan Guangdong, Federasi Asosiasi Ilmu Pengetahuan Perusahaan Industri Makanan dan Kemasan Guangzhou bersama dengan beberapa perusahaan dan institusi, diadakan di Hotel Meilihao, Panyu, Guangzhou. Acara ini mengusung tema "
Hubungi kami untuk mendapatkan penawaran
Untuk sampel, harga, atau dukungan teknis, hubungi kami atau tinggalkan pesan dan kami akan segera membalas.
+86 15916881866 Hubungi kami