国望フォーラム・質問にお答えします・QQグループの質問
- 两层复合膜的油墨和胶水厚度约为1丝,即10μm,而干式复合中油墨与胶水总厚度有接近10μm的说法,也有人认为最多3μm。
- 胶水厚度可按涂布量估算:每1g/m²胶水涂布量增加1μm厚度。
- 对于-4℃冷冻、约200g、袋型22*18cm的去骨鸭掌,建议结构包括NY//PE和NY//RCPP,PET/PE成本较低但在薄规格下存在破袋风险。
- 速冻切鸡可用单层PE表面印刷,总厚度140μm并使用耐冻油墨;鸭掌包装一侧40μm偏薄,至少60μm会更好。
- 使用Nordmeccanica无溶剂复合设备时,每卷膜有数米不固化。
Yongsheng Packaging - Julia: For a two-layer laminated film, apart from the thickness of the film materials, roughly how thick are the ink and adhesive?
Shanghai Yiguang Packaging Equipment: About 1 si, that is, 10um.
Yongsheng Packaging - Julia: For a four-layer structure laminated three times, is it about 3um added for ink and adhesive?
Dong, Guangzhou Tongze Machinery: I think they should be calculated separately, based on the coating weight of ink and adhesive; each 1g/m² of adhesive applied increases thickness by 1um.
Engineer Li: For dry lamination, the total thickness of ink and adhesive should be close to 10um.
Xiao Ke, Jinan: How could it be that thick? At most 3um.
- Frozen Packaging Structure for Duck Feet
Zhongbu Printing: For frozen food bags for duck feet, with deboned duck feet and water inside, stored at -4℃, what structure is suitable? OPP//PE or nylon//PE, or another structure? 40um on one side.
Harbin Botai: Nylon//PE! PE is more suitable for frozen packaging; CPP is too brittle at low temperatures. How heavy is the content?
Song Kai, Guangzhou Bostik: I suggest NY//RCPP.
Zhongbu Printing: Estimated 200g, bag size 22*18cm.
Harbin Botai: If you want premium quality, NY//PE; if you want cost control, single-layer PE with surface printing.
Zhongbu Printing: That makes sense; 40um on one side is a bit thin.
Harbin Botai: Quick-frozen cut chicken all uses single-layer PE, 140um total, with freeze-resistant ink for surface printing.
Zhongbu Printing: How about OPP//frozen PE?
Harbin Botai: No, you can try PET/PE; low cost and decent results.
Zhongbu Printing: Will PET//PE side seams crack at low temperatures, since PET is also brittle?
Xiao Xia, Hubei Dry Lamination: Your structure is not reliable; the PE is a bit thin.
Zhongbu Printing: Which structure is not reliable? The customer wants it thin to save cost.
Harbin Botai: At least 60um would be better.
Xiao Xia: If that's the case, just use 10um nylon.
Zhongbu Printing: Where can I buy 10um nylon?
Xiao Xia: If you want it even cheaper, use 15um OPP.
Zhongbu Printing: What are the pros and cons of PET//PE?
Xiao Xia: PET is fine too, but its density is a bit higher. Calculate which is cheaper; it's really hard to say at this thickness—there is a risk of breakage.
- Solventless Lamination Not Curing
A Flexible Packaging Company: With Nordmeccanica solventless lamination equipment, several meters of each film roll do not cure—sometimes in the middle of the roll, sometimes at the edge. The uncured width is about 4~5cm. What is the cause?
Song Kai, Yidebang Adhesive: It is caused by too long a stoppage in the middle of the run.
A Flexible Packaging Company: Why?
Song Kai: When the machine stops, the adhesive inside the static mixer has already been mixed together; over time it begins to react and its viscosity increases. By the time it is pumped out the second time, the adhesive at the front is not mixed evenly enough, causing local non-curing. Choosing a solventless adhesive with a long pot life can overcome this problem.
A Flexible Packaging Company: But it is not that there is too little adhesive—it does not cure. When torn open there is adhesive, but it just does not cure. The stoppage was just a roll change.
Song Kai: The non-curing phenomenon is caused by uneven mixing of the A and B components—there is no NCO component.
Dong Wentao, Guangzhou Tongze: Are the temperatures set the same for the A and B adhesive tanks?
A Flexible Packaging Company: No, B is 40℃, A is 30℃.
Dong Wentao: At room temperature, is B adhesive more viscous or A adhesive?
A Flexible Packaging Company: B adhesive. There are 7 rolls of material in total; some rolls have two sections that do not cure, while some rolls have only one section that does not cure.
Dong Wentao: Then it may be that the adhesive output is not synchronized.
Song Kai: The core in the middle of the static mixer was installed backwards; it rotates as the adhesive is pumped.
Dong Wentao: Clean the adhesive output pipeline.
A Flexible Packaging Company: It can't be installed backwards. Do you mean the core of the adhesive mixer rotates?
Dong Wentao: Clean the A adhesive pipeline, including the mixing head.
A Flexible Packaging Company: Okay.
Song Kai: Yes.
- Ink Peeling
Lanhai Printing: When printing BOPP heat-seal film with high-temperature ink, some ink still peels off onto the heat-sealing knife of the packaging machine and sticks to it. What is the cause? How can it be solved?
Harbin Botai: Is Teflon tape applied to the heat-sealing knife? It still feels like the ink is not temperature-resistant.
Xiao Ke, Jinan: Generally, designs are not recommended at the sealing position.
Color Printing & Aluminum Coating Consultant: Inks used for printing on OPP are not resistant to high temperatures; temperature-resistant inks generally require high-temperature baking or are two-component.
- Wrinkles in Lamination Winding
Xin, Dalian Jutong Plastics: May I ask, how can wrinkles caused by lamination winding be controlled?
Fl, Dongguan Jinheng Packaging: They can be controlled by adjusting the winding curve of the equipment.
Liu, Xiamen Jinyuan: Adjust the winding tension.
Walking My Own Road: It is poor control of winding tension.
Chengdu Color Printing Management: Are they wrinkles at the bottom of the laminated roll or surface wrinkles?
Xiao Xia: Soft wrinkles.
Yang, Guangzhou Dry Lamination: If the take-up can be run manually, run it manually; once adjusted, do not increase it again, and minimize the number of stoppages.
Lida: Automatic winding tension is indeed rather difficult to control. Tension and the winding curve should be adjusted according to the width and thickness of the film.
Wang, Jinyu Packaging: Winding wrinkles include bottom-of-roll wrinkles, splice wrinkles and surface wrinkles. Bottom-of-roll wrinkles are controlled by initial tension, the tension taper curve setting, a large paper core, and the regularity and smoothness of the paper core; for splice wrinkles, pay attention to the flatness of the splice tape and the rationality of tension switching (equipment performance); surface wrinkles are mostly related to bottom-of-roll wrinkles in the raw material, especially thick film—pay attention to early roll-change splicing.
Gazing at the Starry Sky: Change the core to a larger one.
- Coffee Packaging Structure
Mr. Hu, Taishan Malaysia: Does anyone know the material specification of the roll film used for Nescafé coffee's automatic inner packaging recently? It is an easy-tear material, and every part can be easily torn.
Packaging Rookie: It is made by extrusion lamination, PET/AC/LDPE-LDPE+AE/AL/EAA-MLLDPE, using twin-screw co-extrusion.
Jiang, Guangdong Lamination: PET//PE//AL//PE//PE.
- Blank Doctor Lines
Yang Zibiao: May I ask everyone, why do blank doctor lines always appear during lamination? The adhesive and the adhesive pan are both clean.
Yang, Wuhan Printing: If there are blank doctor lines, it is definitely not clean.
Xiao Xia: Check the blade edge—what adhesive are you using?
Yang Zibiao: Lihe.
Yang, Wuhan Printing: If it always appears, it should not be the blade.
Xiao Xia: Have you used alcohol-soluble and water-based adhesives?
Yang Zibiao: The adhesive is not dirty—no, I haven't; the doctor blade is also quite normal.
Xiao Xia: If it always appears, you need to check whether the blade edge has been wiped clean.
Yang Zibiao: It has been wiped clean.
Liu Liufang: It may be the rubber roller.
Xiao Xia: Put stockings over both ends of the adhesive suction pipe, and rub the blade edge with sandpaper.
Yang, Wuhan Printing: It is definitely caused by debris; find a way to filter the adhesive.
Yang Zibiao: We add adhesive manually. Why should the blade edge be rubbed with sandpaper?
Xiao Xia: If you add adhesive manually, you should store the adhesive properly yourself! Cover it with a lid to reduce dust ingress.
Yang Zibiao: The adhesive is not dirty; it is clean.
Xiao Xia: Why rub the blade edge with sandpaper? To prevent dried adhesive under the blade edge from softening again in the adhesive.
Jingbao—RH: Adjust the doctor blade angle and filter the adhesive. Xiao Xia makes sense.
Yang, Wuhan Printing: Clean thoroughly before use, and filter with a 120-mesh or finer filter screen before use.
Jiangxi Yunlong Color Printing: The adhesive must contain particles; pay attention to the blade angle.
Xiao Xia: A blank doctor line means there is impurity!
Jiangxi Yunlong Color Printing: The anilox roller should also be wiped clean.
Yang Zibiao: The blade angle is basically parallel.
Xiao Xia: You can check for yourself—is there a lot of impurity in the adhesive left in the pan at the end of the shift?
Yang Zibiao: We use a 140-mesh filter screen; after work there is a little impurity in the adhesive.
Xiao Xia: Lower the adhesive pan a bit.
Jiangxi Yunlong Color Printing: There is too much old adhesive stuck under the blade.
Jingbao—RH: There is definitely impurity; the only way to keep impurity from getting stuck in the doctor blade is to adjust the doctor blade angle.
Xiao Xia: If you are in the same workshop as printing, it is best to use fewer poor-quality blankets.
Yang Zibiao: There is no adhesive under the blade; the new machine has only run a few times.
Yang, Wuhan Printing: Find a way to filter the adhesive.
Jingbao—RH: In spring, floating dust, catkins and fibers are all impurities—they can give you a headache.
Engineer Li: Change the blade first and see; go from simple to complex. Then check the thickness and position of the lines and whether continuity changes. Try changing the pressure roller.
Zhang, Shangpin Printing: I think the working concentration of the adhesive is a bit high, and there is impurity in the adhesive; add solvent to reduce the concentration.
(Note: The above are some technical questions discussed in the group. Readers who have different opinions or additions are welcome to submit to us: fanjunhong@126.com or ss8996@126.ccom. You are also welcome to join our flexible packaging technical exchange QQ groups: Main Group: 121451012; Group I: 64311965; Group II: 37848282; Group III: 119411638; Group IV: 116162302; Group V: 256925591).
関連資料
- 選果ラインから凍結乾燥工場まで:食品機械が紡ぐ四川・重慶レモンの深加工チェーン2026-11-27Industry Newsソース: 食品机械设备网·资讯
四川省と重慶市は中国国内の主要なレモン産地であり、中でも四川省安岳県と重慶市潼南区は広く知られている。しかし長らくの間、両地域のレモンの多くは青果として域外に販売され、そのサイズと果皮の外観が販売価格を直接左右していた。深加工の割合は低く、外観が平均的な加工用レモンは低価格でしか販売できないことが多く、ひどい場合には畑で腐ってしまうことさえあった。 小さなレモンからより高い付加価値を生み出す鍵は深加工にあり、このチェーンのあらゆる工程には食品機械のサポートが欠かせません。選別・等級分け:まず原材料を区分する
- 消費者向け環境最適化月間|プラスチック製食品関連製品の購入・使用のヒント2026-11-26Industry Newsソース: 食品伙伴网
食品関連プラスチック製品とは、樹脂または熱可塑性材料を主原料とし、食品や食品添加物の包装・保持に使用され、食品の生産・販売過程において食品に直接接触する製品をいう。中国では、食品用プラスチック包装、容器、工具などの製品に生産許可制度を適用しており、企業は生産・販売活動を開始する前に生産許可証を取得しなければならない。 消費者が利用する一般的なプラスチック製食品関連製品には、メラミン製食器、使い捨てプラスチック製品などがある
- UPM、アジア太平洋地域のラベル材料の生産能力を増強2026-11-26Industry Newsソース: Packaging News Australia
UPM Adhesive Materialsは、マレーシアのジョホールバルにあるラベル材料工場への大規模投資を完了し、アジア太平洋地域での成長を支えるため、生産能力と効率を向上させました。改修された工場には、先進的なコーティングラインが導入され、後加工、梱包、materials搬送能力が強化されています。
- 知能が産業をエンパワー・産学連携イノベーション|2026年産学連携イノベーションイベントAI特別セッションが広州で開催2026-11-24Industry Newsソース: 食品机械设备网
11月17日から18日まで、中国科学技術協会と中華全国工商業連合会が主催し、中国科学技術協会企業革新サービスセンター、中華全国工商業連合会宣伝教育部・経済サービス部が運営を担い、広東省食品・包装機械工業協会、広州市食品・包装業企業科学協会連合会が複数の企業・機関と共同で実施した2026年産業イノベーション協働革新イベントのAI特別セッションが、広州番禺のメリハオホテルで開催された。本イベントは「