  • 本标准规定了瓦楞纸板边压强度试验方法,适用于单瓦(三层)、双瓦(五层)和三瓦(七层)瓦楞纸板。
  • 试样为矩形,尺寸为(25±0.5) mm×(100±0.5) mm,瓦楞方向沿短边;除非双方另有约定,至少裁取10个试样,并按GB 450取样、按GB 10739调节温湿度。
  • 固定压板电子压缩试验机的移动压板速度为(12.5±2.5) mm/min,压板平行度误差不超过1:1000,横向移动不超过0.05 mm。
  • 弯曲梁式压缩试验机在压板接触试样后压力应以(67±13) N/s上升,破坏时读数须在仪器可测变形范围的20%-80%,且其结果不得用于仲裁测试。
  • 测试时试样置于下压板中心且短边垂直于两压板,两个横截面20 mm×20 mm、长度小于100 mm的抛光金属导向块用于保持垂直;压力接近50 N时移除导向块,继续加载至试样破坏,记录最大压力并精确到1 N,边压强度以N/m报告。

This standard sets out the test method for edgewise crush strength in corrugated fibreboard.

It covers single-wall (three-layer), double-wall (five-layer) and triple-wall (seven-layer) corrugated fibreboard for edgewise crush strength measurement.

2 Normative references

When the following documents are cited in this standard, their clauses become part of this standard. The editions listed were valid when the standard was published. Since standards are revised over time, users should examine whether the newest editions below may be used.

GB 450-89 Sampling of paper and paperboard specimens

GB 10739-89 Standard atmosphere for conditioning and testing of pulp, paper and paperboard specimens

3 Test principle

A rectangular corrugated fibreboard sample is placed between the two platens of a compression tester. Its flute direction must be perpendicular to the platens. Pressure is applied until the sample collapses, and the maximum pressure it can bear is measured.

4 Test apparatus

4.1 Fixed-platen electronic compression tester

This unit has one fixed platen and one platen that is directly and rigidly driven. The moving platen speed is (12.5±2.5) mm/min. Platen dimensions must match the selected sample size so the sample does not extend past the platens. The platens must also meet these conditions:

a) parallelism error of the platens: no more than 1:1000;

b) lateral movement: no more than 0.05 mm.

4.2 Bending-beam compression tester

This tester uses the beam-bending principle. Its upper and lower platens must satisfy the same requirements as the fixed-platen electronic compression tester. At the moment of collapse, the reading must be within 20%-80% of the instrument's measurable deflection range. Once the platens touch the sample, pressure should rise at (67±13) N/s.

When this instrument is used, the report must state that fact, and the results must not be used for arbitration testing.

4.3 Sample cutting device

Samples may be prepared with a band saw, knife or die, but the cut edges must be smooth, straight and perpendicular to the board surface.

4.4 Guide blocks

Two polished rectangular metal blocks, each 20 mm×20 mm in cross-section and under 100 mm long, hold the sample in place and keep it perpendicular to the platens.

5 Sampling and conditioning of samples

5.1 Sample collection must follow GB 450.

5.2 Samples must be conditioned for temperature and humidity as specified in GB 10739.

6 Sample preparation

Cut rectangular samples so that the flute direction lies along the short side; dimensions are (25±0.5) mm×(100±0.5) mm. Samples must have no indentations, printing marks or damage. At least 10 samples must be cut unless both sides agree otherwise.

7 Test procedure

Cutting and testing must take place under the atmospheric conditions given in 5.2.

Position the sample in the centre of the lower platen so its short side is perpendicular to both platens. Use guide blocks to support it, keeping its end faces perpendicular to the platens; the two guide blocks must be parallel to each other and perpendicular to the sample surface.

Switch on the tester and apply pressure. When pressure nears 50 N, take away the guide blocks and keep loading until the sample collapses. Record the maximum pressure the sample can withstand, rounded to 1 N.

Test the remaining samples in the same way.

8 Expression of results

Edgewise compressive strength is calculated with formula (1) and reported in N/m:

Where: R —— edgewise compressive strength, N/m;

F —— maximum pressure, N;

L —— long-side dimension of the sample, mm.

9 Test report

A test report needs to cover the following:

a) the number of this national standard;

b) sample type and specification;

c) the standard applied in the test;

d) atmospheric conditions at the test site;

e) tester model and loading speed;

f) arithmetic mean of the test results;

g) other data that helps clarify the test results.

Source: China Packaging Network (pack.cn), original link: http://news.pack.cn/show-362290.html

संबंधित लेख

  • छँटाई लाइनों से लेकर फ्रीज-ड्राई कार्यशालाओं तक · …
    2026-11-27Industry Newsस्रोत: 食品机械设备网·资讯

    सिचुआन और चोंगक्विंग घरेलू स्तर पर प्रमुख नींबू उत्पादक क्षेत्र हैं, जहां सिचुआन का आन्यू और चोंगक्विंग का तोंगनान व्यापक रूप से प्रसिद्ध हैं। हालांकि, लंबे समय से इन दोनों क्षेत्रों के अधिकांश नींबू ताजे फल के रूप में बाहर भेजे जाते रहे हैं, जिनका आकार और छिलके का बाहरी स्वरूप सीधे विक्रय मूल्य को निर्धारित करता है। गहन प्रसंस्करण का अनुपात कम था, और सामान्य दिखावट वाले प्रसंस्करण योग्य नींबू अक्सर कम कीमत पर ही बिक पाते थे, यहां तक कि खेतों में ही सड़ जाते थे। छोटे नींबू से उच्च मूल्य संवर्धन प्राप्त करने की कुंजी गहन प्रसंस्करण में निहित है, और इस श्रृंखला का प्रत्येक चरण खाद्य मशीनरी के समर्थन के बिना कार्य नहीं कर सकता। छंटाई और ग्रेडिंग: कच्चे माल को सबसे पहले विभाजित करें

  • उपभोक्ता वातावरण सुधार माह | प्लास्टिक खाद्य उत्पादों की खरीद और उपयोग के लिए सुझाव
    2026-11-26Industry Newsस्रोत: 食品伙伴网

    खाद्य से संबंधित प्लास्टिक उत्पादों में प्लास्टिक पैकेजिंग, कंटेनर और उपकरण शामिल हैं, जिनकी मुख्य कच्ची सामग्री रज़िन या थर्मोप्लास्टिक सामग्री होती है, जिन्हें भोजन या खाद्य योजक को पैकेज करने और रखने के लिए उपयोग किया जाता है और जो भोजन के उत्पादन और संचालन के दौरान भोजन के सीधे संपर्क में आते हैं। चीन खाद्य-उपयोगी प्लास्टिक पैकेजिंग, कंटेनर, उपकरण और अन्य उत्पादों के लिए उत्पादन लाइसेंस प्रबंधन लागू करता है, और उद्यमों को उत्पादन और संचालन में शामिल होने से पहले उत्पादन लाइसेंस प्राप्त करना आवश्यक है। उपभोक्ताओं द्वारा उपयोग किए जाने वाले सामान्य प्लास्टिक खाद्य-संबंधी उत्पादों में मेलामिन टेबलवेयर, फेंकने योग्य प्लास्टिक शामिल हैं।

  • UPM ने एशिया-प्रशांत में लेबल सामग्री की क्षमता में वृद्धि की
    2026-11-26Industry Newsस्रोत: Packaging News Australia

    यूपीएम एडहेसिव मटेरियल्स ने मलेशिया के जोहोर बहरू में अपने लेबल सामग्री कारखाने में बड़ा निवेश पूरा कर लिया है, जिससे एशिया-पैसिफिक में विकास को समर्थन देने के लिए उत्पादन क्षमता और दक्षता में वृद्धि हुई है। उन्नत किए गए इस कारखाने में अत्याधुनिक कोटिंग लाइन तथा बेहतर पोस्ट-प्रोसेसिंग, पैकिंग और सामग्री संचालन क्षमताएं हैं।

  • इंटेलिजेंस उद्योग को सशक्त बनाता है · उद्योग-नवाचार सहयोग | गुआंगज़ौ में आयोजित 2026 उद्योग-नवाचार सहयोगी · …
    2026-11-24Industry Newsस्रोत: 食品机械设备网

    17 से 18 नवंबर तक, चाइना एसोसिएशन फॉर साइंस एंड टेक्नोलॉजी और ऑल-चाइना फेडरेशन ऑफ इंडस्ट्री एंड कॉमर्स द्वारा आयोजित, चाइना एसोसिएशन फॉर साइंस एंड टेक्नोलॉजी के एंटरप्राइज इनोवेशन सर्विस सेंटर, ऑल-चाइना फेडरेशन ऑफ इंडस्ट्री एंड कॉमर्स के प्रचार एवं शिक्षा विभाग और आर्थिक सेवा विभाग द्वारा संचालित, तथा गुआंगडोंग फ़ूड एंड पैकेजिंग मशीनरी इंडस्ट्री एसोसिएशन, गुआंगज़ौ फ़ूड एंड पैकेजिंग इंडस्ट्री एंटरप्राइज साइंस एसोसिएशन फेडरेशन द्वारा कई उद्यमों और संस्थानों के साथ संयुक्त रूप से कार्यान्वित 2026 उद्योग-नवाचार सहयोगी नवाचार कार्यक्रम का एआई विशेष सत्र गुआंगज़ौ के पान्यू में मेइलिहाओ होटल में आयोजित किया गया। यह आयोजन "" की थीम पर आधारित है

उद्धरण के लिए हमसे संपर्क करें

नमूनों, मूल्य या तकनीकी सहायता के लिए हमें कॉल करें या संदेश छोड़ें और हम जल्द ही उत्तर देंगे।

+86 15916881866 संपर्क करें